Saturday, January 28, 2012

Dyeing process of Lycra Single Jersey Fabric

Learn Apparel Merchandising, Learn Fashion design.
Single Jersey Spandex (Lycra) Fabric

Dear All, 

Today I will share with you a very important dyeing process. Some times we got query from buyer for Fabric with spandex. All of these the most common require fabrication is - 95% cotton 5% spandex, Single jersey  , 160 GSM. From the fiber market we can got many kinds spandex for knitting the fabric. Denier is the unit of Spandex. The common denier is 20D, 40D & 70D. Fiber thickness of 20D is thin then 40D. And 70D is thicker then 40D. Lycra is a brand (name) of Spandex.  

In single jersey spandex fabric it is very difficult to keep the GSM lower. If you intending to produce the s/j cotton spandex fabric in between 155 to 165 GSM then please follow the below things:

Fabric 95% cotton 5% spandex, Single Jersey, 160 GSM

Yarn count should be - 40/s comb
Spandex should be - 20D
Stitch Line should be - 2.80

Dyeing Process of Single Jersey Cotton Spandex Fabric:

  • 1st step: After receive the grey fabric from knitting section in tube form, in dyeing section, at first we slit the fabric by slitting machine. 
  • 2nd Step: Then we heat set the slitted fabric by stenter machine for avoiding the creased mark. And also for the Dia & Grey GSM fixing.

          Dyeing the fabric (in the winch)-
    • Option A) If the dyeing factory has high pressure dyeing machine (winch) then we should dye the fabric in open width. 
    • Option B) If the dyeing factory has normal dyeing winch then we should back sewing the open fabric to make it tube again.
  • 3rd Step: Scouring (detergent wash) the fabric in the dyeing winch and released the water for perform the next process. 
  • 4th Step: Labeling the fabric by labeling agent which increased the PH of fabric.
  • 5th Step: Soda / Salt wash.
  • 6th Step: Mixing the specific color (reagent) for dye the fabric. Or if fabric color is white then we used brightener chemical in this step. And step 06 is not require for white color fabric.
  • 7th Step: Acid wash (after released color mixing water) 
  • 8th Step: Color fixing by fixer. 


          Finishing process of the fabric (After dyeing) -


          If we are following option (A) then step will be like as below
  • 9th Step: Stentering (heat setting) for adjust the Dia. For this again stentering we called it double heat settings. 
  • 10th Step: Open compacting for control shrinkage of fabric length.   
            
          If we are following option (B) then step will be like as below
  • 9th Step: Slitting 
  • 10th Step: Stentering (heat settings) for dia adjust.
  • 11th Step: Open compacting for control shrinkage of fabric length. 

Now the fabric is ready for cutting. Please test the Shrinkage, Color shade, Gsm before start cutting.
Hope, it will be helpful for all of you


Thanks & best regards
Bipul

8 comments:

  1. what would be the care instructions and symbols for 95% ciscose 5% spandex single jersey 290 gsm tshirt ?

    ReplyDelete
  2. Hi!
    I want to know the care symbols and instructions for 290 gsm 95% viscose 5% lycra t shirt.

    ReplyDelete
  3. If you need big quantities meltblown nonwoven fabric, it will be a good choice to buy a meltblown material, it will be more cost-effective for a long-term profit.

    ReplyDelete
  4. Very good points you wrote here..Great stuff...I think you've made some truly interesting points.Keep up the good work. Bayern Munich Jersey Online

    ReplyDelete
  5. Belgium Home Jersey 2022 has a red color with black raglan sleeves with flame graphic rising up from the end of the sleeves. The stripes on the shoulders are red, as is the new logo, while the badge has shiny gold finish.

    ReplyDelete





Related Posts Plugin for WordPress, Blogger...